Aluminium-Killed Steels | ||||||||||||
Design. | SEBIR Nr. | Description | Applications | Recommended Austenizing and tempering temperature | Class 8.8 | Class 9.8 | Class 10.9 | Class 12.9 | Class 8.8 | Class 9.8 | Class 10.9 | Class 12.9 |
Quenching Medium: | OIL (Index H= 0.40) | WATER (Index H= 0.2) |
||||||||||
1.0303 | 015 | C4C | Oil-quenched heat treatments not supported | Not supported |
||||||||
1.0213 | 011 | C8C | Untreatable steels |
|||||||||
1.0214 | 056 | C10C | ||||||||||
1.0234 | 005 | C15C | Simple hardenability steels | 865-900º + 445-505ºC | Water quenched supported |
|||||||
1.0411 | 058 | C20C | ||||||||||
1.0501 | 733 | XC35 | 835-865º + 500-600ºC | |||||||||
1.1061 | 009 | C45 RC | Hardening steel | |||||||||
1.1192 | 010 | C45 EC |
ACEROS AL BORO | ||||||||||||
Design. | SEBIR Nr. | Description | Applications | Recommended Austenizing and tempering temperature | Class 8.8 | Class 9.8 | Class 10.9 | Class 12.9 | Class 8.8 | Class 9.8 | Class 10.9 | Class 12.9 |
Quenching Medium: | OIL (Index H= 0.40) | WATER (Index H= 0.2) |
||||||||||
1.5502 | 001 | 17B2 | 860-890º + 450-500ºC | ≤M6 | ≤M8 | |||||||
1.5508 | 004 | 22B2 | ≤M8 ≤M3 | ≤M14 ≤M10 | ||||||||
1.5514 | 022 | 33B2 | 835-865º + 450-550ºC | ≤M10 ≤M10 ≤M5 ≤M3 | ≤M25 ≤M20 ≤M12 ≤M5 | |||||||
1.5515 | 706 | 36B2 | ≤M12 ≤M10 ≤M10 ≤M5 | |||||||||
1.5525 | 306 | 20MnB4 | 860-890º + 450-550ºC | ≤M8 ≤M3 | ≤M14 ≤M10 | |||||||
1.5537 | 309 | 36MnB4 | 835-865º + 450-550ºC | ≤M16 ≤M14 ≤M12 ≤M10 | ||||||||
B Cr STEELS |
||||||||||||
1.5522 | 307 | 22MnB4Cr | Improved hardenability steels for quenching and tempering | 860-890º + 450-550ºC | ≤M12 ≤M10 ≤M3 | ≤M25 ≤M20 ≤M60 | ||||||
1.5515 | 312 | 36MnB4CR | 835-865º + 450-550ºC | ≤M12 ≤M10 ≤M10 ≤M5 |
BORON STEELS WITH CR CONTENT OF 1% |
||||||||
Design. | SEBIR Nr. | Description | Applications | Recommended Austenizing and tempering temperature | Class 8.8 | Class 9.8 | Class 10.9 | Class 12.9 |
Quenching Medium: | OIL (Index H= 0.40) |
|||||||
1.7076 | 102 | 32CrB4 | High hardenability steels for quenching and tempering | 835-865º + 500-600ºC | ≤M12 ≤M12 ≤M12 ≤M12 | |||
1.7077 | 104 | 36MnB4 |
ALLOY STEELS WITH CR AND OTHER ALLOYS |
||||||||
Design. | SEBIR Nr. | Description | Applications | Recommended Austenizing and tempering temperature | Class 8.8 | Class 9.8 | Class 10.9 | Class 12.9 |
Quenching Medium: | OIL (Index H= 0.40) |
|||||||
1.7034 | 703 | 37Cr4 | High hardenability and standard strength steels | 835-865º + 500-600ºC | ≤M18 ≤M15 ≤M12 ≤M10 | |||
1.7035 | 012 | 41Cr4 | ≤M20 ≤M18 ≤M15 ≤M14 | |||||
1.7039 | 019 | 41CrS4 | ≤M25 ≤M22 ≤M20 ≤M14 | |||||
1.7243 | 402 | 18CrMo4 | High hardenability and improved strength steels | 865-900º + 445-505ºC | ≤M6 | |||
1.7220 | 003 | 34CrMo4 | 835-865º + 500-600ºC | ≤M18 ≤M16 ≤M15 ≤M10 | ||||
1.7202 | 705 | 37CrMo4 | ≤M25 ≤M20 ≤M18 ≤M12 | |||||
1.7225 | 008 | 42CrMo4 | ≤M30 ≤M25 ≤M20 ≤M18 | |||||
1.7227 | 059 | 42CrMoS4 | ≤M35 ≤M30 ≤M25 ≤M22 |
OTHER APPLICATIONS |
|||
Design. | SEBIR Nr. | Description | Applications |
1.7131 | 054 | 16MnCr5 | Cementation |
1.7711 | 401 | 40CrMoV4-6 | High temperature ch4 |
1.3505 | 742 | 100Cr6 | Ball bearing |
1.0718 | 034 | F210E | Free cutting |
1.0403 | 407 | C15Pb | |
1.0503 | 717 | C42C | Nails |
1.0613 | 718 | C62C |